Key takeaways
- A clear guide to tadelakt plaster on an approved bathroom feature wall, from substrate checks and mixing to two-coat application, stoning, soaping and care.
As an Amazon Associate I earn from qualifying purchases. This post may contain affiliate links at no extra cost to you.
A bathroom feature wall finished in tadelakt carries a warmth that paint and tile rarely match. The surface holds a soft, cloudy shine, the colour sits deep in the plaster rather than on top of it, and the wall feels smooth and cool to the hand. The word tadelakt comes from the Arabic verb for rubbing or kneading, and the name describes the work itself: lime plaster rubbed and burnished with a stone until the pores close and the surface turns water repellent. How to apply tadelakt plaster on an approved bathroom feature wall is a question that starts long before the first trowel of plaster, because the finish only performs when the wall beneath it has been checked, accepted and prepared in the right way.
An approved wall means a substrate that the plaster maker accepts for tadelakt. The ideal base is brickwork carrying at least 1.5 cm of hydraulic lime plaster or lime-cement plaster, untreated and solid, with a rough open surface that the fresh plaster can grip. Plasterboard, gypsum plaster, concrete and cement fibre board can also carry tadelakt, but only after priming with a casein primer and an intermediate coat of lime wall finish with a glass fibre net embedded in it. A feature wall in a bathroom sits in a splash zone rather than a direct water zone, which matters: the maker of Kreidezeit Tadelakt states clearly that the plaster suits decorative surfaces in splash water areas and is not recommended for showers, wash basins and bathtubs. Longer-moistened areas absorb water and darken temporarily, then brighten again as they dry. A feature wall behind a freestanding bath or beside a vanity, where water reaches it only as occasional splashes, sits comfortably inside that guidance, while a wall inside a shower enclosure does not.
Tadelakt is a demanding craft technique, and the maker says so plainly. Good craftsmanship and experience are essential to achieve the characteristic appearance and a sound functional surface. That should not put a careful first-timer off, but it does set the pace of the job: work in small sections, keep the plaster from drying too fast, and give each stage the time it needs. A feature wall is a sensible first large surface because it is flat, visible, and usually free of the pipework and corners that complicate a shower wall. The reward for patience is a finish with no grout lines, no visible joints and a depth of colour that changes gently as daylight moves across the room.
Quick answer
Start with a substrate that has been checked and accepted for tadelakt, then prime absorbent surfaces and lay an intermediate lime coat with embedded glass fibre net where the maker requires it. Mix the dry powder with 0.25 litres of clean cold water per kilogram, rest the mix for about 30 minutes, stir again, and use it within 8 to 10 hours. Apply two thin coats, each about 1 to 1.5 mm, burnish the second coat with a polishing stone in small circles until the pores close and gloss appears, then soap the surface while it is still a little moist. Soap a second time after the surface has dried completely, within two days at most. Allow 2 to 3 days for the wall to dry at 3 mm of layer thickness, handle it gently for the first 3 months, and expect full hardness after about 6 months.
| Item | What it does | When to use it |
|---|---|---|
| Kreidezeit Tadelakt | Mineral lime plaster for the two finish coats | The main plaster for the feature wall |
| Marius Fabre Savon Noir | Black olive oil soap for the soaping stage | First and second soaping, and later aftercare |
| Kreidezeit Tadelakt Polishing Stone ST177 | Hardened ceramic stone that closes pores and builds gloss | Burnishing the second coat and working soap into the surface |
| Kreidezeit Casein Primer | Colourless primer that evens out suction on absorbent substrates | Before the intermediate coat on plasterboard, gypsum or concrete |
| Kreidezeit Pigments | Mineral pigments for tinting the plaster | When the wall needs a colour other than natural white |
| Refina SUPERFLEX-2 | Flexible stainless finishing trowel for flattening coats | Laying and closing the two tadelakt coats |
Step by step
1. Confirm that the wall is approved for tadelakt
Read the wall before touching a bag of plaster. The substrate must be dry, rough, solid, clean and free of grease, dust and loose material. Run a hand across it: a sound lime plaster base feels open and slightly sandy, while a smooth painted surface feels closed and slick. Tadelakt must not be applied onto smooth surfaces, and sharp edges in the plaster should be rounded because the thin coats cannot hide a hard arris and the stone cannot burnish around one. Check for hollow spots by tapping; any drummy area needs cutting out and repair with similar material before the job starts. On board substrates, check that every board is fixed solidly and that joints are filled and flat, because movement in a board shows through two coats that together measure only about 3 mm.
Approval also means matching the wall to the plaster. Brickwork with at least 1.5 cm of hydraulic lime plaster or lime-cement plaster takes tadelakt directly. Gypsum plasters, lime-gypsum plasters, concrete, plasterboards, gypsum fibre boards, Wedi Boards and cement fibre boards need priming with Casein Primer or Vega Primer followed by an intermediate coat of Lime Wall Finish -medium- with a glass fibre net embedded in it, and the net must be covered completely. On clay plasters in dry areas, the maker recommends pre-hardening with potassium waterglass diluted 1 part waterglass to 3 parts water, with at least 24 hours of drying, then primer and the same intermediate coat. If the wall carries old distemper, chalking paint or wallpaper glue, remove it thoroughly; a coat of tadelakt cannot bond to a failing layer beneath it. Where the wall sits beside a bath or basin, confirm that the area is a splash zone and not a zone of standing water, since tadelakt is not suitable on continuously moist surfaces.
2. Prime the substrate and lay the intermediate coat
Where the substrate needs it, prime first. Kreidezeit Casein Primer arrives as a powder: add 250 g to 3 litres of clean cold water while stirring constantly, let it expand for about 30 minutes, stir again thoroughly, then dilute with 5 litres of water. Apply the primer evenly and saturated with a brush, using only as much liquid as the substrate absorbs, and wipe away any wet glossy spots with a cloth before drying. Do not spray it and do not apply it with a roller. The primer dries after about 8 hours at 20 degrees Celsius and is then safe to coat with lime or casein based materials. One 250 g pack covers about 40 to 60 square metres depending on absorbency, so a single feature wall needs only a small part of a pack. The primer must be used on the same day it is mixed, and primer that smells bad or rotten must never be used, since the odour can linger even after drying. Application temperature must stay above 8 degrees Celsius.
Over the primer, lay the intermediate coat of Lime Wall Finish -medium-, article number 960, with a glass fibre net embedded across the whole board area. The net spreads stress and reduces the risk of shrinkage cracking in the thin finish coats above it. Keep the coat even and cover the net fully, then let it dry completely before the tadelakt goes on. On a solid lime plaster base that needs no primer, the intermediate coat is unnecessary; the tadelakt can be applied directly onto the rough lime surface once it is dry and sound. Either way, dampen the subsurface lightly before plastering, because a thirsty base pulls water out of the first coat too fast and leaves a weak bond.
3. Mix the plaster to the right consistency
Tadelakt is a dry powder made of hydraulic lime, quartz sands, marble powder, clay and methylcellulose, with no cement and no artificial contents. Stir the dry powder gradually into the given amount of clear, cold water, using a powerful electric drill with a paint stirrer. The maker lists 0.25 litres of water for 1 kilogram of powder, and the amount of water can be increased slightly if necessary. After an expanding period of about 30 minutes, stir again thoroughly. Mixed tadelakt must be used within 8 to 10 hours, so mix only as much as the next section of wall needs. Coverage runs at 2.5 kilograms per square metre at 2 mm of thickness, which means a 2.5 kilogram bag covers about 1 square metre, a 10 kilogram bag about 4 square metres, and a 25 kilogram bag about 10 square metres. Measure the wall, add a small allowance for the sample panel and for waste at edges and corners, and choose bag sizes that match the area rather than opening a large bag for a small wall.
Mixing matters more than it looks. Lumps in the mix become hard spots in the finish, and a mix that is too wet slumps and dries with a weak surface. Stir the powder in gradually rather than dumping it in at once, scrape the rim of the bucket from time to time with a trowel, and whisk again if the mix has stood for 30 minutes. Keep the bucket covered between mixes so the surface does not skin over. Protect the fresh plaster from drying too fast during application: avoid draughts, high temperatures and direct sunlight, and close the bathroom door and window while working if the room runs hot or dry.
4. Tint the plaster before the first coat
Kreidezeit Tadelakt is naturally white and can be tinted with up to 10 percent of Kreidezeit pigments by weight, so 10 kilograms of tadelakt can take up to 1 kilogram of pigment. Tinting with titanium white and pure iron oxide pigments is limited to 5 percent. Stir the pigments with a little water to a paste first, making sure all clots are stirred out properly, then stir the pigment paste into the mixing water before adding the tadelakt powder. The paste can also be added to the ready-mixed plaster mass, but mixing it into the water first gives a more even colour. Demineralised water gives the best results for dissolving pigments. Mix thoroughly to achieve even tinting, and clean the rim of the bucket from time to time with a trowel so dried pigment does not fall back into the mix as dark specks.
Colour discipline decides whether the wall reads as one surface. Mix the full quantity of tinted plaster for the whole wall in one batch where the wall size allows it, and weigh the pigment rather than judging by eye. If the wall needs more than one batch, weigh each batch identically and keep a note of the weights, because a small difference in pigment shows as a band across the wall once the surface is burnished. Do not store tadelakt pigmented with ultramarine pigments for longer than 24 hours. A sample panel in the chosen colour, finished through stoning and soaping, shows the true colour far better than a wet patch on the wall, since the soap deepens the tone and the burnish changes how light sits on the surface.
5. Apply the first coat thinly and leave it alone
Apply the first layer with a trowel entirely and only slightly thicker than the grain size, about 1 to 1.5 mm. The maker is explicit on this point: the first layer must not be smoothed, polished or densified, and it should not dry completely before the second layer goes on. Its job is to key the second coat and to even out the suction of the substrate, not to look finished. Lay it with the Refina SUPERFLEX-2, using the flexible 0.4 mm blade to spread the plaster in even passes without pressing hard. Let the first coat set until the surface has become strong against impact. On a small feature wall the wait is usually an hour or two, but the exact time depends on the water content of the surface, its absorbency and the climate of the room, so read the surface rather than the clock.
Work in sections that one person can finish in a single session, because both tadelakt layers and the first treatment with soap must be performed within the same day. A feature wall of three to four square metres is a comfortable single-day section for a careful worker. Keep edges wet where a new section meets the last one, and avoid leaving a hard dry edge in the middle of the wall, since the joint will show after burnishing. Wet dry subsurfaces before application, and keep the room free of draughts while the coats set.
6. Apply the second coat and burnish it with the stone
Apply the second layer with a trowel entirely and only slightly thicker than the grain size, again about 1 to 1.5 mm, and let it set. Flat surfaces can be pre-densified with a trowel, and a plastic smoothing spatula helps to flatten the surface and close small holes before the stone comes out. Then burnish the surface while moving the Kreidezeit Tadelakt Polishing Stone ST177 in small circles with only light pressure, until all pores are closed and gloss is achieved. The right moment for pre-densifying and burnishing depends on the water content of the surface, its absorbency and the climate, and it can vary strongly, so check a small area first: rub it with the stone, and if no plaster comes off on the stone and the surface turns shiny where the stone has passed, the moment has arrived. If plaster sticks to the stone, wait longer. If the surface has dried too far, the stone slides without closing the pores, and the gloss stays patchy.
Burnishing is the heart of tadelakt. The stone compresses the aggregate, closes the pores and creates the smooth, softly undulating shine that gives the finish its character. Work in small circles with light, even pressure, overlapping each pass, and keep the stone clean. The circular polishing movements produce the typical slight cloudiness of the surface, which is part of the look rather than a fault. Corners and edges need the same attention as the flat field, and the stone follows curves that a trowel cannot, which is why tadelakt suits rounded reveals and soft arrises. Take time here: the gloss built now decides how the wall reads for years.
7. Soap the surface twice, then wax only the dry areas
The first layer of soap should be applied shortly after burnishing the second tadelakt layer, while the surface is still a little moist and has not dried completely. Dilute the soap in a ratio of 1 part soap to 6 parts water, and never use the concentrate undiluted. Brush the solution evenly over the surface with a soft brush, working in sections of about 1 square metre, and remove any surplus with the brush. Let it set a short while, then burnish with the polishing stone until a regular gloss appears. For this article the soap is Marius Fabre Savon Noir, a black olive oil soap: potassium based, liquid or paste, highly concentrated and most often used diluted, made from vegetable oils including olive oil. The chemistry is the same as with any olive soap on fresh lime: part of the natural soap changes into lime soaps that give the wall surface moisture and dirt repellent properties, a process that makes the finish water repellent rather than merely water resistant.
After the surface has completely dried, and no later than after 2 days, apply the soap solution again. Let it set a short time, then polish the surface with a ball formed out of plastic foil. Aftersoaping keeps the function of the surface in wet areas: repeat the diluted soap treatment every 1 to 2 months, and polish with the plastic foil ball after a short setting time. Waxing is optional and comes only after the surface is completely dry. Use wax only on soaped surfaces, and do not use wax in areas affected by water splashes, because white stains can appear. On a feature wall the dry upper band can take a thin coat of wax polished with a clean soft cloth for a higher gloss, while the lower band near the bath stays soap finished only.
8. Let the wall dry, harden and settle
Tadelakt dries after 2 to 3 days at 3 mm of layer thickness. Treat the surface gently within the first 3 months, and the final hardness will be achieved after about 6 months. During that period the wall is still gaining strength, so avoid leaning objects against it, avoid scrubbing, and wipe away water splashes with a soft cloth after every use so limescale does not build. Once a day the wall should dry completely; if tadelakt stays moist for too long, matt areas, discolouration and fungi can occur, which is another reason the finish belongs on a feature wall rather than inside a shower.
Cleaning stays simple for the life of the wall. Clean tadelakt surfaces only with water with a little Marseille soap or Corfu soap added, about 1 to 2 spoons per 8 litres of water, using a soft sponge. Do not use other household cleaning agents, scouring sponges or microfibre cloths, since they can mark the burnished surface or strip the soap finish. Keep the room ventilated so the wall dries between uses, and keep a small bottle of diluted soap ready for the monthly aftersoap. A wall cared for in this way keeps its shine and its water repellent surface for years, and a small mark can be repaired by cutting out the damage and patching with the original material.
Tools and materials
Kreidezeit Tadelakt
- Dry powder; bags of 2.5 kg, 10 kg and 25 kg
- Coverage 2.5 kg per square metre at 2 mm; 2.5 kg covers about 1 square metre
- Two layers, each about 1 to 1.5 mm; water 0.25 litres per 1 kg of powder
- Rest about 30 minutes after mixing; use within 8 to 10 hours
- Naturally white; tintable with up to 10 percent Kreidezeit pigments
- pH above 12.5; sd-value below 0.1 m; free of cement; purely mineral
- Composition: hydraulic lime, quartz sands, marble powder, clay, methylcellulose
Kreidezeit Tadelakt is the plaster itself, and its data sheet sets the rules for the whole job. The thin two-layer build, the short working window after mixing, and the demand that both layers and the first soaping happen on the same day all come from the maker, not from habit. The plaster is water resistant as mixed, and the final treatment with an olive oil soap makes the surface water repellent through a reaction between the soap and the fresh lime. On a feature wall the plaster shows its best side: a warm, velvety surface with a soft cloudy shine from the circular polishing movements, and a colour that sits inside the material.
Pros: Maker data covers mixing, layers, drying and care in full; thin build suits a feature wall; wide colour range from mineral pigments.
Cons: Demanding technique with a same-day schedule; not suitable for showers, basins, tubs or floors; needs gentle handling for 3 months.
Marius Fabre Savon Noir
- Black olive oil soap; potassium based, liquid or paste form
- Highly concentrated; most often used diluted
- 100 percent natural; ECOCERT certified; no colourants, perfume, palm oil, solvent or preservative
- Dark brown colour from olive pomace oil
- Formats of 500 ml pump, 1 litre and 5 litres
- Maker founded in 1900 in Salon-de-Provence
Savon Noir is the traditional black soap of the tadelakt trade, and it earns its place here because the soaping stage is where the finish becomes water repellent. The soap is made from vegetable oils including olive oil, turned to soap with a potassium base, which makes it soft and highly concentrated. Diluted 1 part soap to 6 parts water, it brushes on evenly and works into the surface under the stone. The same soap serves for the monthly aftersoap that keeps the finish working, so one bottle covers both the job and its care.
Pros: Traditional olive oil soap for tadelakt; concentrated, so a small bottle goes far; doubles as the aftercare soap.
Cons: Must always be diluted; dark colour needs care on very pale plaster until the dilution is right.
Kreidezeit Tadelakt Polishing Stone ST177
- Hardened ceramic; hardness grade 9.5 on the Mohs scale
- Pore-free surface; ergonomically shaped for hand use
- Used by hand with polishing soap in small circular motions
- Closes pores and builds gloss on the second coat
- Also used to work the soap into the surface after soaping
The polishing stone is the tool that turns two thin coats of plaster into tadelakt. A steel trowel can flatten, but only a smooth hard stone compresses the aggregate and closes the pores to the point where the surface shines. The ST177 is formed from hardened ceramic, so its face stays smooth and pore-free, and its ergonomic shape suits hours of small circular movements. The readiness check is simple and reliable: rub a small area with the stone, and if no plaster comes off and the surface shines where the stone passed, the wall is ready for soap.
Pros: Purpose made for burnishing; pore-free ceramic face; ergonomic shape for long sessions.
Cons: Works only at the right moment in drying; a stone used too early picks up plaster.
Kreidezeit Casein Primer
- Article number 1103; powder for mixing with water
- Mix 250 g into 3 litres of cold water, rest about 30 minutes, dilute with 5 litres
- 250 g covers about 40 to 60 square metres depending on absorbency
- Dried after about 8 hours at 20 degrees Celsius
- Colourless and transparent; sd-value below 0.01 m; free of preservatives
- Composition: casein, sodium carbonate
- Apply with a brush; do not spray and do not use a roller; minimum 8 degrees Celsius
Casein Primer evens out the thirst of the substrate so the intermediate coat and the tadelakt dry at the same rate across the wall. Without it, a patch of highly absorbent plasterboard drinks the water from the first coat while a denser patch beside it stays wet, and the finish dries in bands. The primer reduces absorbency, compensates for differences between areas, and slightly solidifies sandy substrates, all without reducing the vapour absorption of the plaster, which matters in a lime system. It suits clay, lime, lime-cement and gypsum plasters, plasterboard, gypsum fibre boards, stone and concrete, and it is the primer the Kreidezeit system names before the intermediate coat.
Pros: Very economical coverage; keeps the lime system vapour open; suits all absorbent substrates in the system.
Cons: Must be used on the same day it is mixed; not suitable on smooth non-absorbent surfaces or permanently moist substrates.
Kreidezeit Pigments
- Mineral pigments for tinting tadelakt and other Kreidezeit plasters
- Up to 10 percent by weight in tadelakt; 10 kg of plaster takes up to 1 kg of pigment
- Titanium white and pure iron oxide pigments limited to 5 percent
- Stir with a little water to a paste before adding to the mixing water
- Demineralised water gives the best results for dissolving pigments
- Do not store plaster pigmented with ultramarine pigments longer than 24 hours
Pigments are what turn a white feature wall into a coloured one, and the discipline around them is weighing, not guessing. The colour deepens under the soap and changes again under the stone, so the only honest colour reference is a finished sample panel. Because the limit is a weight percentage, a kitchen scale and a notebook matter as much as the trowel: record the pigment weight per bag, mix the whole wall from one batch where possible, and keep the same ratio across batches when the wall needs more than one.
Pros: Wide colour range from mineral sources; colour sits inside the plaster rather than on the surface.
Cons: Small weighing differences show as bands; ultramarine mixes have a 24 hour storage limit.
Refina SUPERFLEX-2
- 0.4 mm stainless steel blade; 120 mm blade width
- Longer bracket gives a slightly stiffer feel than the SUPERFLEX-1
- Balance of flexibility and control for flattening and finishing
- Rounded corners and finished blade edges help reduce drag marks
- Flexible construction for controlled finishing passes
The SUPERFLEX-2 is the laying and closing trowel for this job. Its 0.4 mm blade flexes enough to follow the wall and close the surface without digging in, while the longer bracket keeps a little more stiffness along the blade than the most flexible model in the range, which helps when the second coat needs a firm, even pass before the stone comes out. Rounded corners and finished edges reduce the drag marks that a sharp corner leaves in a thin lime coat. It is a finishing trowel, not a laying-on trowel for heavy coats, and on tadelakt that distinction suits the work, since each coat measures only about 1 to 1.5 mm.
Pros: Good balance of flex and control for thin coats; clean edges reduce drag marks.
Cons: Not made for laying on heavy coats; the blade needs cleaning between passes to avoid dragging residue.
Common mistakes
Skipping the primer and intermediate coat on board substrates
Tadelakt laid straight onto bare plasterboard or gypsum plaster dries unevenly and bonds poorly. The board drinks water from the first coat in patches, the finish sets in bands, and the bond fails where suction was highest. Prime with casein primer, lay the intermediate lime coat with embedded glass fibre net, let it dry fully, and only then start the tadelakt. The extra day saves the wall.
Mixing a batch too large for one section
Mixed tadelakt must be used within 8 to 10 hours, and both layers plus the first soaping belong to the same day. A batch mixed for the whole wall when only half can be laid in the session ends as waste in the bucket, and worse, a batch used past its working life lays poorly and stones badly. Measure the section, weigh the powder for that section, and mix again for the next one.
Working the second coat after it starts to set
The second coat has a window: firm enough to hold the trowel, still moist enough to close under the stone. Working it after it has started to set tears the surface, leaves drag lines, and opens pores that the stone cannot close again. Watch the surface, not the clock, and if a section has gone past its window, leave it and return to the sequence on the next section rather than forcing the trowel through a setting coat.
Stoning or soaping too late
Burnishing and soaping both depend on moisture in the surface. Stone too late and the pores stay open; soap too late and the soap sits on a dry surface instead of reacting with the fresh lime. The first soaping belongs shortly after burnishing, while the plaster is still a little moist, and the second soaping belongs after complete drying and within two days at most. Keep the sequence tight and keep the room free of draughts so the timing stays in hand.
Waxing the splash zone or waxing before the surface is dry
Wax belongs only on soaped surfaces that are completely dry, and never in areas affected by water splashes, where white stains can appear. On a feature wall the lower band near the bath is a splash zone even when it looks dry, so keep the wax to the dry upper band and leave the lower band soap finished. Waxing a damp surface seals moisture in and clouds the finish.
FAQ
Can tadelakt go inside a shower?
Kreidezeit Tadelakt is not recommended for showers, wash basins and bathtubs, and the maker states this plainly. The plaster suits decorative surfaces in splash water areas, while longer-moistened areas absorb water and darken temporarily. A shower wall needs a plaster whose maker rates it for direct wet areas, together with a waterproofed substrate and an intermediate coat. A feature wall outside the shower enclosure is the right place for this plaster.
How much plaster does a feature wall need?
Coverage runs at 2.5 kilograms per square metre at 2 mm of thickness, so a 2.5 kilogram bag covers about 1 square metre, a 10 kilogram bag about 4 square metres, and a 25 kilogram bag about 10 square metres. Measure the wall, allow a little extra for the sample panel and for waste at edges and corners, and weigh the water at 0.25 litres per kilogram of powder. Two coats at about 1 to 1.5 mm each make up the 2 to 3 mm total build.
How long before the wall can be used normally?
The wall dries after 2 to 3 days at 3 mm of layer thickness, and the second soaping should be finished within 2 days of the first. Treat the surface gently for the first 3 months, avoid leaning objects against it and avoid scrubbing, and expect full hardness after about 6 months. Light use of the bathroom can resume once the wall is dry and soaped twice, but the finish keeps gaining strength for months.
Why does the surface darken when it gets wet?
Tadelakt is water resistant rather than completely impermeable, and a longer-moistened area absorbs water and becomes dark temporarily. The maker notes that this is normal and that the surface brightens again once dry. Wiping splashes away with a soft cloth after use keeps the darkening brief, and the monthly aftersoap keeps the water repellent surface working. Persistent dark patches that do not brighten after drying point to a spot where the soap finish is thin and need a fresh aftersoap.
Can the colour be matched if a repair is needed later?
Colour matching starts at mixing time: weigh the pigment for every batch, record the weight per bag, and keep a small sealed sample of the dry pigmented powder. A repair cut from the same batch and finished with the same stoning and soaping will blend far better than a repair mixed by eye. Small repairs can be made by cutting out the damage and patching with the original material, then stoning and soaping the patch to match the surrounding gloss.
Conclusion
A tadelakt feature wall rewards a methodical job: an approved substrate, a primer and intermediate coat where the system requires them, a weighed mix, two thin coats laid on the same day, careful burnishing with the stone, and two soapings inside two days. The plaster itself is simple in composition, hydraulic lime, quartz sands, marble powder, clay and methylcellulose, and the finish comes from craft rather than from additives: the stone closing the pores, the olive soap reacting with the fresh lime, and the slow hardening that follows over months. Keep the wall out of direct shower water, soap it every month or two, clean it only with a little Marseille or Corfu soap in water, and the surface will hold its warm shine and its water repellent skin for years. The feature wall is the right place to learn the technique, and a wall finished this way gives the bathroom a surface with no grout lines, no visible joints, and a depth of colour that paint cannot match.
Related guides
More ways to save on your next finish
Programs that pair well with the guide above. Offers and eligibility are set by Amazon and may change.
A free business account with business pricing and bulk-buying tools for work, shop or home office.
Create a business accountFast, free shipping on eligible items, plus Prime Video and more. Eligible new members can start with a free trial.
Start a Prime free trialRead from a huge library of eBooks, including how-to guides and cookbooks. Eligible new members can start with a free trial.
Try Kindle UnlimitedAudiobooks and podcasts for the commute, the garage or the kitchen. Eligible new members can start with a free trial.
Try Audible freeAs an Amazon Associate we earn from qualifying purchases. Using these links costs you nothing extra.
Write Your Review
No reviews yet. Be the first to share your experience!