Updated Th11 26, 2026· 21 min read

Key takeaways

  • Learn how to apply lime-based stucco on traditional brickwork with a breathable NHL 2 system, from preparation and three coats to floating, curing and care.

As an Amazon Associate I earn from qualifying purchases. This post may contain affiliate links at no extra cost to you.

Traditional brickwork asks for a finish that works with the wall rather than against it. Old bricks are soft, porous, and full of small variations in firing, and the mortar joints between them move a little with every change of season. A hard, dense coating traps water behind the face, forces salts toward the surface, and pushes the outer skin of the brick away in thin flakes. How to apply lime based stucco on compatible traditional brickwork starts from that single fact: the coating must breathe, flex a little, and stay weaker than the brick it covers.

Lime-based stucco does all three when the mix is right. Natural hydraulic lime sets by a slow reaction with water and then continues to harden by taking carbon dioxide from the air, a process that leaves a network of fine pores open. Water vapour passes through, the wall dries after rain, and salts stay in solution instead of crystallising behind a sealed skin. The work itself follows a calm, old rhythm: dampen the wall, throw on a haired scratch coat, rule it flat, let it firm up, add a float coat, then finish with a thin coat that a sponge float brings to a soft, even face. Nothing in the sequence needs force or speed. Each coat needs time, water, and a steady hand.

This guide walks through the full job on a compatible traditional brick wall, meaning a wall built with soft, low-fired bricks laid in lime mortar, with no cement render and no paint film left on the face. The system below uses natural hydraulic lime grade NHL 2 as the binder, a one-layer lime render for dubbing out, washed sharp sand as the aggregate, goat hair as the reinforcement, a glass fibre mesh over joints and repairs, and a golden stainless finishing trowel for the final pass. Every material and every figure in this guide comes from a maker data sheet or a trade guide that has been opened and read.

Quick answer

Apply lime-based stucco to compatible traditional brickwork in three coats over a dampened, well-keyed face. Rake out loose joints, wet the wall until it stops drinking, then throw on a haired NHL 2 scratch coat about 10 mm thick and scratch it for a key. After the scratch coat firms up, apply a float coat of the same mix, rule it flat, and finish with a thin 5 mm coat of NHL 2 and fine sand, worked with a sponge float. Keep every coat damp for several days, protect the work from sun, wind, and frost, and never use cement anywhere in the build-up.

Item What it does When to use it
NHL 2 site-mixed stucco Soft, breathable three-coat system matched to old brick Full wall, traditional build-up, maximum control over mix
Fassa FASSACOUCHE one-layer render Air lime render applied in one thicker layer Dubbing out hollows and uneven brickwork before the finish
Pre-blended lime render Factory-mixed lime and aggregate, steady quality Large areas where a uniform mix matters more than site mixing
Lime putty finish Fine, fat lime coat for a smooth face Final coat on sheltered walls where a soft finish suits the brick
Mesh over joints and repairs Glass fibre mesh that bridges movement and cracks Over repaired joints, cracks, and changes of material

Step by step

1. Read the wall before touching it

Walk the whole wall face and look at the brick first. Compatible traditional brickwork shows soft arrises, a slightly uneven face, and mortar joints that yield to a fingernail or a blunt screwdriver. Press a thumb against a joint: lime mortar crumbles a little and feels sandy, while cement mortar stays hard and grey. Tap the face with a knuckle and listen for hollow spots where an old render has parted from the brick. Mark every hollow area, every crack wider than a hairline, and every patch of paint, bitumen, or cement pointing with chalk. A wall that still carries a cement render or a plastic paint film is not compatible until those layers come off, because they block the very movement of vapour that lime stucco depends on.

Check the brick for salts as well. White fluffy deposits on the face point to soluble salts in the wall, and a lime finish will not cure that problem on its own. Brush the salts off dry, find the source of the water, and let the wall dry as far as the season allows before starting. Look at the plinth, the sills, and the ground level too: a wall that sits in splash from a hard paving or a broken gutter will wet through no matter how good the stucco is, so fix the water path first. Note the exposure of the wall face as well. A south-facing wall in open sun dries fast and needs more misting, while a shaded north wall stays damp longer and needs more time between coats.

2. Prepare the surface and open a key

Rake out every loose or powdery joint to a depth of about 15 to 20 mm, using a plugging chisel and a club hammer, and take care not to chip the brick arrises. A joint that is sound and well filled can stay, but any joint that falls away under a light scrape has to go, because a stucco coat cannot bond to dust. Cut back any proud cement pointing and remove paint or bitumen with a stiff wire brush and a scraper; where a paint film clings hard, a steam stripper or a poultice softens it without driving water deep into the brick. Brush the whole face down with a stiff bristle brush to clear dust, cobwebs, and loose crumbs, then wash the wall with clean water from a hose at low pressure. High-pressure washing drives water into the brick and can cut the soft face, so keep the jet gentle and the distance generous.

Dampen the wall thoroughly before any stucco goes on, and do it twice. The first wetting goes on the evening before the work or at least an hour ahead, so the brick drinks its fill and the surface stops pulling water from the mix. The second wetting goes on just before the first coat, enough to darken the face evenly without leaving water running down the joints. A wall that is too dry will suck the water out of the fresh coat and leave it powdery and weak; a wall that is running wet will let the coat slide and slump. The right state is a face that looks evenly dark and feels cool and damp to the back of the hand, with no standing water in the joints.

3. Mix the NHL 2 scratch coat

Natural hydraulic lime grade NHL 2 is the binder for this job, and its data sheet sets the terms. St Astier NHL 2 comes in 25 kg bags, meets the EN 459 standard, carries a strength factor of 2, and shows a whiteness index of 76. The finish coat ratio is 1 part lime to 2.5 parts sand at about 5 mm, the initial set takes 5 to 6 hours, the coat can be reworked within 24 hours, and the fresh work needs protection for 96 hours. Working temperature sits between 8 and 30 degrees Celsius, which means no lime work in frost and no lime work on a wall baking in hot sun.

Mix the scratch coat at 1 part NHL 2 to 2.5 parts washed sharp sand graded 0 to 3 mm, with natural goat hair added at 5 to 10 kg per cubic metre of mortar. Washed sharp sand suits this coat because the grains are angular and clean, and the guidance from trade sources is clear that building sand has no place in lime render. The sand must be washed and graded, not dug soft sand, because clay and silt in the aggregate weaken the set and stain the face. Add the hair to the dry mix first and turn it through so the strands separate, then add clean water a little at a time and mix until the mortar holds together on the trowel without slumping. A paddle mixer keeps the hair evenly spread; hand mixing on a board works too if the hair is teased apart before the water goes in. The finished mortar should feel fatty and a little sticky, firm enough to throw, and wet enough to key into the joints.

4. Throw on the scratch coat and scratch a key

Load the hawk, take a trowel full of mortar, and throw it at the wall with a firm flick of the wrist so the mortar drives into the joints and the pores of the brick. Work from the bottom of the lift upward, covering about a square metre at a time, and press the coat into the face with the flat of the trowel after the first throw. The scratch coat should land about 10 mm thick, even across the face, with no thin spots where the brick shows through. Where the wall steps back or a joint runs deep, dub out the hollow first with the same mix and let it firm before the main coat goes over it.

Once the coat has stiffened enough to hold a mark without tearing, drag a scratch comb or a lath across the face in a loose diamond pattern, cutting lines about 3 mm deep and 25 mm apart. The key gives the next coat something to grip, and the diamond pattern spreads the grip evenly in every direction. Do not scratch while the coat is still soft and wet, or the lines will close up again; do not wait until it has set hard, or the comb will drag and tear. On a mild day the right moment comes a few hours after the coat goes on, when a thumb pressed lightly into the surface leaves a print without sinking. Leave the scratched coat alone after that. It needs days, not hours, and the next coat must wait until the scratch coat has firmed right through.

5. Dub out hollows with the one-layer render

Before the float coat, walk the wall again and look for hollows, bellies, and places where the brickwork steps in or out. A straightedge held against the face shows every dip at once. Dub out the deep spots with Fassa FASSACOUCHE, an air lime one-layer render whose data sheet calls for a first layer of at least 10 mm sprayed or thrown from the bottom upward, with a sponge float finish within 24 hours. The sheet also warns not to wet the surface or touch it up after application, which matters because rewetting a one-layer render can lift the skin and leave a weak, dusty face.

Apply the dubbing in layers no thicker than the sheet allows, and let each layer firm before the next goes on. Press the render into the hollow with the trowel, rule it back to the line of the wall, and leave the surface rough so the float coat can grip. Over a repaired joint or a crack, bed a strip of Fassa FASSANET 160 glass fibre mesh into the first pass of render. The mesh weighs 160 grams per square metre, resists alkali attack from the lime, and sits over joints and irregular substrates to spread movement instead of letting it open as a crack. Lap each strip at least 100 mm past the repair on both sides, and keep the mesh buried in the middle of the coat, not floating on the surface where it can show through the finish.

6. Apply the float coat and rule it flat

Dampen the scratch coat lightly before the float coat goes on, just enough to darken it without leaving free water. Mix the float coat at the same ratio as the scratch coat, 1 part NHL 2 to 2.5 parts washed sharp sand, but leave the hair out of this coat. The float coat carries the flatness of the wall, so it goes on a little thicker than the finish, about 8 to 10 mm, thrown on in the same way and then ruled with a straightedge. Work the straightedge in a slow sawing motion across the face, first in one direction and then at a slight angle, cutting the high spots and filling the low ones with the mortar the edge carries.

Let the float coat firm up, then work it with a wooden float in small circular movements to close the surface and bring the sand grains to an even texture. The float coat is the layer that decides how flat the finished wall looks, so take time here and check with the straightedge again after the first floating pass. Any hollow that still shows gets a thin dub of the same mix, pressed in and ruled flat before the surface firms. Keep the wall damp while the float coat firms, misting lightly with a sprayer whenever the surface starts to pale. A float coat that dries too fast will craze with a network of fine cracks, and those cracks will show through the finish coat no matter how carefully it goes on.

7. Finish with a thin coat and float it to a soft face

The finish coat uses the same NHL 2 binder at 1 part lime to 2.5 parts sand, laid about 5 mm thick, which matches the data sheet figure for the finish coat. Dampen the float coat first, then trowel the finish on in a thin, even layer, working from the bottom of the lift upward and keeping a wet edge so one section flows into the next without a dry joint. A dry joint in the finish shows as a pale line that no amount of floating will hide, so plan the lifts around the natural breaks in the wall, such as a string course, a plinth, or a corner, and finish each lift without stopping.

When the finish has firmed enough to take a float without tearing, work it with the sponge float in slow circular movements, using the Marshalltown MXS64GSD finishing trowel first to close the surface if the trowel leaves a mark. The MXS64GSD carries a 14 by 4 inch golden stainless steel blade, hardened and tempered, with a curved DuraSoft handle and an aluminium alloy Xtralite mounting, and the bevelled work edges let the blade close the surface without digging in. The sponge float then brings the face to a soft, even texture with the fine sand showing as a gentle grain. Keep the float damp, rinse it often, and change the water when it turns milky, because dirty water drags lime across the face and leaves pale streaks.

After the finish, the wall needs care for days. Mist the surface lightly two or three times a day for at least four days, and hang damp hessian over the face if the sun or the wind is strong. The data sheet calls for 96 hours of protection for NHL 2, and that figure is a minimum rather than a target: cool, damp weather is a friend to lime, and a slow, even set gives a stronger, more durable face. Keep frost off the work entirely, and do not paint or seal the stucco until it has dried right through, which can take several weeks on a thick build-up.

Tools and materials

St Astier NHL 2 natural hydraulic lime

St Astier NHL 2 is a soft natural hydraulic lime in 25 kg bags, made to the EN 459 standard with a strength factor of 2 and a whiteness index of 76. The maker data sheet gives an initial set of 5 to 6 hours, reworking within 24 hours, protection for 96 hours, and a working range of 8 to 30 degrees Celsius. The finish coat ratio is 1 part lime to 2.5 parts sand at about 5 mm thick. Grade 2 is the softest hydraulic class, which is why it suits old brick: it stays weaker than the brick, lets vapour through, and moves a little with the wall instead of fighting it.

  • 25 kg bag; EN 459; strength factor 2; whiteness 76
  • Finish coat 1:2.5 lime to sand at about 5 mm
  • Initial set 5 to 6 hours; rework within 24 hours; protect 96 hours
  • Working temperature 8 to 30 degrees Celsius

Pros: Softest hydraulic grade, well matched to old brick; long working time; pale colour that suits a lime finish.
Cons: Slow to gain strength, so the wall needs longer protection; not suited to very exposed or frost-prone work without shelter.

Fassa FASSACOUCHE one layer lime render

Fassa FASSACOUCHE is an air lime render designed to go on in one thicker layer rather than three thin ones. The maker data sheet calls for a first layer of at least 10 mm, applied from the bottom upward, with a sponge float finish within 24 hours, and it warns not to wet the surface or touch it up after application. That single-layer behaviour makes it the right material for dubbing out hollows and for bringing an uneven brick face back to a true line before the finish coat.

  • Air lime one-layer render; first layer minimum 10 mm
  • Apply from the bottom upward; sponge float finish within 24 hours
  • Do not wet or touch up after application

Pros: Builds thickness in one pass; good for dubbing out; air lime stays very breathable.
Cons: Needs care with timing, since the finish window is fixed; rewetting after application can lift the skin.

Marshalltown MXS64GSD Finishing Trowel

The Marshalltown MXS64GSD is a finishing trowel with a 14 by 4 inch golden stainless steel blade, hardened and tempered, a curved DuraSoft handle, and an aluminium alloy Xtralite mounting. The bevelled work edges let the blade close a lime finish without digging lines into the surface, and the golden stainless face resists rust and stays smooth through a long day of floating. At 14 inches long and 4 inches wide it covers ground quickly on a flat wall while staying light enough for overhead work.

  • 14 x 4 in golden stainless steel blade, hardened and tempered
  • Curved DuraSoft handle; aluminium alloy Xtralite mounting
  • Bevelled work edges; limited lifetime warranty

Pros: Long blade closes a large area fast; golden stainless stays smooth and rust-free; comfortable handle for long sessions.
Cons: A 14 inch blade needs a steady hand on small or broken surfaces; the price sits above a plain carbon steel trowel.

Fassa FASSANET 160 alkali resistant glass fibre mesh

Fassa FASSANET 160 is a glass fibre mesh weighing 160 grams per square metre, made to resist alkali attack from lime. The maker guidance places it over joints and irregular substrates, embedded in the first coat, with the second layer going on once the first has set. On old brickwork it bridges repaired joints, cracks, and places where one material meets another, spreading small movements across the mesh instead of letting them open as a single crack in the finish.

  • 160 g/m2 alkali resistant glass fibre mesh
  • Embed over joints and irregular substrates
  • Second layer once the first has set

Pros: Spreads movement and helps avoid cracking over repairs; alkali resistant, so lime does not weaken it.
Cons: Must sit buried in the coat, not on the surface; a mesh line left proud will show through the finish.

Washed sharp sand 0 to 3 mm

Washed sharp sand graded 0 to 3 mm is the aggregate for the scratch and float coats in this system. Trade guidance gives washed graded sharp sand in the 0 to 5 mm or 0 to 3 mm range, mixed at 1:2.5 to 1:3 with NHL 3.5, and the same ratios serve NHL 2. The grains are angular and clean, which gives the mortar body and a key, and the washing removes clay and silt that would weaken the set and stain the face. Building sand, which is soft and rounded, has no place in this work.

  • Washed graded sharp sand, 0 to 3 mm
  • Mix 1:2.5 to 1:3 with NHL
  • Angular clean grains; not building sand

Pros: Clean angular grains give body and a good key; grading suits scratch and float coats.
Cons: Must be washed and graded, which costs more than dug sand; a wrong grading changes the finish texture.

Natural goat hair

Natural goat hair is the traditional reinforcement for a lime scratch coat on weak substrates, added at 5 to 10 kg per cubic metre of mortar in the scratch coat only. The hair spreads through the mix and holds the coat together while it firms, which matters on old brick where the face is uneven and the suction varies from brick to brick. Trade guidance puts goat hair or polypropylene fibre in the scratch coat on weak substrates, in base coats only, and the old rule still holds: hair belongs in the first coat, where it does its work out of sight, not in the finish.

  • 5 to 10 kg/m3 in scratch coat on weak substrates
  • Base coats only; not for the finish coat
  • Haired scratch coat thrown or laid on masonry and scratched for a key

Pros: Traditional reinforcement that suits old work; holds a thick scratch coat together; cheap for the strength it adds.
Cons: Needs even spreading through the mix or it clumps; adds a step to the mixing that a plain mix skips.

Common mistakes

Using cement anywhere in the build-up

Cement is the most common and most damaging mistake on old brickwork. A cement scratch coat, a cement gauged mix, or even a cement wash under the lime creates a hard, dense layer that traps water and forces salts to crystallise behind the face. The lime coats above it cannot breathe through the cement, so the wall stays wet, the brick face flakes, and the lime coat parts from the wall in sheets. Keep cement out of the mortar, out of the dubbing, and out of the pointing that sits behind the stucco.

Applying stucco to a dry wall

A dry brick face drinks the water out of the fresh coat before the lime can set, leaving a powdery, weak skin that dusts off under a finger. The wall must be dampened the evening before or at least an hour ahead, and again just before the coat goes on, until the face darkens evenly and stops pulling water. On a hot day, mist the wall again between lifts, and keep a sprayer at hand through the whole job.

Laying one thick coat instead of three

A single coat 25 mm thick will slump, crack as it dries, and bond poorly to the brick. Lime stucco works as a system: a haired scratch coat for grip, a float coat for flatness, and a thin finish coat for the face. Each coat must firm before the next goes on, and each coat should stay within the thickness its data sheet allows. A thick single coat also dries unevenly, with the face setting while the back stays soft, which opens shrinkage cracks that run right through to the brick.

Letting the coats dry too fast

Sun, wind, and low humidity pull water from a fresh lime coat faster than the lime can use it, and the result is a face full of fine crazing. Mist the work two or three times a day for at least four days, hang damp hessian over the wall face when the weather turns dry or windy, and plan the work for mild, overcast days where the choice exists. A slow set is a strong set, and the extra days of aftercare cost nothing against the cost of redoing a cracked wall face.

Skipping mesh over repairs and joints

A repaired joint, a filled crack, or a change from brick to stone moves differently from the wall around it, and a lime coat laid straight over the joint will crack along the same line. Bed a strip of glass fibre mesh into the first coat over every repair, lap it at least 100 mm past the repair on both sides, and keep it buried in the middle of the coat. Mesh left on the surface shows through the finish, and mesh left out entirely leaves the crack to return.

Floating the finish too early or too late

A finish coat floated while it is still soft tears and drags, leaving trowel marks and soft ridges that never flatten out. A finish floated after it has set hard will not move at all, and the float will burnish the face into a hard, shiny skin that cracks later. The right moment comes when a thumb pressed lightly into the surface leaves a print without sinking, and the float moves in slow circles without dragging the coat. Judge by feel, not by the clock, because temperature and humidity change the timing from day to day.

FAQ

Can lime-based stucco go over old cement render?

No. Cement render must come off before lime stucco goes on, because the cement layer blocks vapour and traps water behind the face. Strip the cement carefully, rake the joints, and let the wall dry before starting the lime work. A wall that keeps any cement pointing behind the stucco will still suffer where the cement sits.

How thick should each coat be?

The scratch coat lands about 10 mm thick, the float coat about 8 to 10 mm, and the finish coat about 5 mm, which matches the NHL 2 data sheet figure for the finish. Dubbing out with the one-layer render starts at a minimum of 10 mm. Keep each coat inside its data sheet thickness, and let each coat firm before the next goes on.

How long does lime stucco take to harden?

The initial set of NHL 2 takes 5 to 6 hours, the coat can be reworked within 24 hours, and the fresh work needs protection for 96 hours. Full hardening by carbonation takes weeks, and the wall should not be painted or sealed until it has dried right through. Cool, damp weather slows the work a little and gives a stronger face.

Why does the scratch coat need hair?

Hair holds the scratch coat together while it firms, which matters on old brick where suction varies from brick to brick and the face is uneven. Goat hair goes in at 5 to 10 kg per cubic metre of mortar, in the scratch coat only, spread evenly through the mix before the water goes in. The finish coat carries no hair, so no strands show on the face.

What sand suits lime stucco on old brick?

Washed sharp sand graded 0 to 3 mm suits the scratch and float coats, mixed at 1:2.5 to 1:3 with NHL. The sand must be washed and graded, with angular clean grains, and building sand has no place in the work because its soft, rounded grains and clay content weaken the set.

Can a beginner do this job?

A careful beginner can do a small, sheltered wall with guidance, but a full wall face on a historic facade is work for a plasterer who has laid lime before. The judgement calls — when the wall is damp enough, when a coat is firm enough to float, how much water the mix needs — come from handling the material. Start on a garden wall or a sample panel, and bring in a specialist for the main wall face.

Conclusion

Lime-based stucco on compatible traditional brickwork succeeds when the system stays softer than the brick, open to vapour, and patient in its timing. NHL 2 gives the right softness for old, low-fired brick, washed sharp sand gives the body, goat hair holds the scratch coat, and a glass fibre mesh bridges the repairs. Three coats, each inside its data sheet thickness, each kept damp while it firms, and each given days rather than hours, add up to a face that dries after rain, moves with the wall, and ages with the building instead of fighting it. Keep cement out, keep the wall damp, and let the lime set at its own pace, and the stucco will serve the brickwork for decades.

A
admin88
We compare specs, warranty terms, long-term owner feedback and street pricing before anything earns a spot. Rankings are never paid.
Affiliate disclosure. As an Amazon Associate we earn from qualifying purchases at no extra cost to you. Prices accurate as of the date shown.

Related guides

Browse all How-to, sửa lỗi & học tập guides →

Handpicked for this guide

More ways to save on your next finish

Programs that pair well with the guide above. Offers and eligibility are set by Amazon and may change.

Most popular
🏢
Amazon Business
Free to sign up

A free business account with business pricing and bulk-buying tools for work, shop or home office.

Create a business account
🚚
Amazon Prime
Free trial for new members

Fast, free shipping on eligible items, plus Prime Video and more. Eligible new members can start with a free trial.

Start a Prime free trial
📖
Kindle Unlimited
Free trial for new members

Read from a huge library of eBooks, including how-to guides and cookbooks. Eligible new members can start with a free trial.

Try Kindle Unlimited
🎧
Audible
Free trial for new members

Audiobooks and podcasts for the commute, the garage or the kitchen. Eligible new members can start with a free trial.

Try Audible free

As an Amazon Associate we earn from qualifying purchases. Using these links costs you nothing extra.